At a glance
Making a spin-coated PDMS layer involves substrate preparation, a sacrificial layer, PDMS spin coating and release of the membrane. The spin-coating speed, acceleration and time define the thickness of the PDMS layer. The process uses a wafer, a spin coater, a hot plate and acetone for the release.
- Wafer preparation
- Heating for 15 min at 120°C in an oven; plasma treatment for 5 min if needed
- Sacrificial layer
- AZ4562 photoresist, baked 2 min at 100°C, no exposure needed
- PDMS mixing ratio
- Monomer to curing agent 10/1, followed by degassing
- Release
- Wafer placed in acetone for 2 to 3 min to dissolve the AZ4562