How to make a PDMS lithography replication from a SU-8 mold
At a glance
Making a PDMS replica from a SU-8 mold involves mold silanization, PDMS mixing, degassing, pouring, baking, peeling, cutting and piercing, and bonding. The mold must first be made hydrophobic by silanization, otherwise the PDMS sticks and peeling becomes impossible, and the PDMS should be weighed before the curing agent is added. Equipment includes a fume hood for silanization, a desiccator with a vacuum pump for degassing, an oven or hot plate for baking, and a plasma cleaner for bonding.
- Mixing ratio
- Sylgard 184: 1:10 curing agent to PDMS (weight), PDMS added first
- Degassing
- Usually 30 minutes in a desiccator under vacuum
- Baking
- Advised: 80°C in an oven for 2 hours; no more than 90°C in a Petri dish
- Plasma bonding
- O2 or air plasma, advised 500 mTorr, 2 minutes, to bond PDMS to glass or PDMS
The 