How to succeed with SU-8 photoresist baking
At a glance
SU-8 photoresist baking involves a soft bake after spin coating, a post exposure bake (PEB) after UV exposure and an optional hard bake. The soft bake evaporates solvent, the PEB supplies the heat energy to continue the reaction activated by UV, and the hard bake relieves stresses that can cause cracks. Uniform heat on a clean, flat and horizontal hot plate and smooth temperature ramps are critical conditions.
- Soft bake solvent content
- Around 7% of solvent enables a good exposure
- Hard bake temperature
- More than 120°C
- Classical temperature ramps
- 10°C per min to increase; 5°C per min to decrease
- Maximal temperatures
- After exposure, transition temperature at 200°C; polymer destroyed after 380°C
SU-8 photoresist baking: pre-bake, soft bake and hard bake